无机盐工业
主管:中海油天津化工研究设计院有限公司
主办:中海油天津化工研究设计院有限公司
   中海油炼油化工科学研究院(北京)有限公司
   中国化工学会无机酸碱盐专业委员会
ISSN 1006-4990 CN 12-1069/TQ

无机盐工业 ›› 2026, Vol. 58 ›› Issue (1): 115-122.doi: 10.19964/j.issn.1006-4990.2024-0689

• 催化材料 • 上一篇    

催化裂化过程中铁的钝化机理及其对催化剂抗铁污染性能的影响

杜晓辉1(), 刘涛1, 薛亚刚2, 王世存2, 高雄厚3()   

  1. 1.中国石油石油化工研究院兰州化工研究中心,甘肃 兰州 730060
    2.中国石油石油化工研究院昆冈 先进制造(北京)有限公司,甘肃 兰州 730060
    3.中国石油兰州石化分公司,甘肃 兰州 730060
  • 收稿日期:2024-12-20 出版日期:2026-01-10 发布日期:2025-08-12
  • 通讯作者: 高雄厚(1963— ),男,博士,教授级高级工程师,研究方向为炼油催化剂新技术、新材料、新工艺;E-mail:gaoxionghou@petrochina.com.cn
  • 作者简介:杜晓辉(1983— ),男,博士,高级工程师,研究方向为炼油催化剂及新材料;E-mail:duxiaohui01@petrochina.com.cn

Passivation mechanism of iron in catalytic cracking and its effect on catalyst′s anti⁃iron contamination performance

DU Xiaohui1(), LIU Tao1, XUE Yagang2, WANG Shicun2, GAO Xionghou3()   

  1. 1. Lanzhou Petrochemical Research Center,Petrochemical Research Institute,PetroChina,Lanzhou 730060,China
    2. Kungang Advanced Manufacturing(Beijing) Co. ,Ltd. ,Petrochemical Research Institute,PetroChina,Lanzhou 730060,China
    3. Lanzhou Petrochemical Company,PetroChina,Lanzhou 730060,China
  • Received:2024-12-20 Published:2026-01-10 Online:2025-08-12

摘要:

以氧化镁、活性氧化铝和硝酸镧为原料,通过喷雾干燥法制备催化裂化金属捕集助催化剂CatClean,以提升催化裂化催化剂的抗铁污染性能,制备的金属捕集助催化剂CatClean主要由质量分数为60%的MgO与质量分数为30%的La2O3组成,磨损指数为1.3%/h。采用浸渍法进行铁污染,在催化裂化催化剂中添加或未添加CatClean的情况下,通过XRD、XPS、NH3-TPD、H2-TPR、EDX-Mapping等方法研究抗铁组分对催化剂反应性能的影响。结果表明:铁污染导致催化裂化催化剂的比表面积显著降低;在高温水热条件下,CatClean中的La2O3与铁反应生成稳定的LaFeO3相,可有效抑制铁对催化剂的负面影响,未观察到MgFe2O4相的生成。EDX-Mapping结果进一步表明,铁元素可在催化剂与CatClean颗粒间迁移并被有效捕集。反应性能评价结果表明,当铁污染量为1.0%(质量分数)时,在反应转化率基本相当的条件下,焦炭产率降低0.78%~0.98%、干气产率降低0.30%~0.33%、总液收增加0.91%~0.95%,显著降低催化剂的副产物选择性,提高催化剂的抗铁污染性能。

关键词: 催化裂化, 金属污染, 氧化镁, 稀土,

Abstract:

To enhance the resistance of catalytic cracking catalysts to iron contamination,a metal⁃trapping additive named CatClean was developed using magnesium oxide(MgO),activated alumina(Al2O3),and lanthanum nitrate[La(NO33] as raw materials via a spray drying method.The resulting CatClean was primarily consist of 60% MgO and 30% La2O3,with a wear index of 1.3%/h.Iron contamination was introduced through an impregnation method,and the effects of CatClean on catalyst performance were systematically investigated using XRD,XPS,NH3-TPD,H2-TPR,and EDX-Mapping techniques.The results indicated that iron contamination significantly reduced the surface area of the catalytic cracking catalyst.Under high⁃temperature hydrothermal conditions,La2O3 in CatClean reacted with iron to form a stable LaFeO3 phase,effectively mitigating the adverse effects of iron:No formation of MgFe2O4 was detected.EDX-Mapping further revealed that iron species could migrate between catalyst and CatClean particles and be effectively captured.Performance evaluations demonstrated that at an iron contamination level of 1.0%,the addition of CatClean reduced the coke yield by 0.78%~0.98%,the dry gas yield by 0.30%~0.33%,and increased the total liquid yield by 0.91%~0.95%,without significantly affecting conversion.These findings confirmed that CatClean significantly reduced the selectivity toward undesired by⁃products and enhanced the catalyst′s resistance to iron contamination.

Key words: catalytic cracking, metal pollution, magnesium oxide, rare earth, iron